ЖC3 Enquiry | Print this page
GOST ЖC3 Details
GOST ЖC3 Standard Download
Category | Type | Grade | Designations |
---|---|---|---|
Grades | Stainless Steels | ЖC3 | Russia - GOST , |
Elements | Min.(≥) | Max.(≤) | Similar | Remarks |
---|---|---|---|---|
C | 0.11 | 0.16 | ||
Cr | 14.00 | 18.00 | ||
Al | 1.60 | 2.20 | ||
Mo | 3.00 | 4.50 | ||
Ti | 1.60 | 2.30 | ||
Co | - | - | ||
W | 4.50 | 6.50 | ||
Ni | - | remaining | ||
Nb | - | - | ||
Fe | - | 8.00 | ||
B | - | 0.02 | ||
Ce | - | - | ||
V | - | 0.30 | ||
Zr | - | - | ||
Mn | - | 0.60 | ||
Si | - | 0.60 | ||
S | - | 0.009 | ||
P | - | 0.015 |
Proof strength Rp0.2 (MPa) |
Tensile strength Rm (MPa) |
Impact energy KV (J) |
Elongation at fracture A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
814 (≥) | 134 (≥) | 44 | 13 | 24 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 231 |
Property | Density kg/dm3 |
Temperature T °C/F |
Specific heat J / kgK |
Thermal conductivity W/mK |
Electric resistance µΩ·cm |
Modulus of elasticity kN/mm2 |
Expansion rate |
---|---|---|---|---|---|---|---|
595 (≥) | 351 (≥) | 32 | 32 | 33 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 143 | |
Temp. °C/°F |
Creep strain limit (10000h) (Rp1,0) N/mm2 |
Creep rupture strength (10000h) (Rp1,0) N/mm2 |
|||||
953 | 964 | 161 |
Product type | Products | Dimension | Processes | Deliver Status |
---|---|---|---|---|
Plates / Sheets | Plates / Sheets | 0.08-200mm(T)*W*L | Forging, hot rolling and cold rolling | Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting |
Steel Bar | Round Bar, Flat Bar, Square Bar | Φ8-1200mm*L | Forging, hot rolling and cold rolling, Cast | Black, Rough Turning, Shot Blasting, |
Coil / Strip | Steel Coil /Steel Strip | 0.03-16.0x1200mm | Cold-Rolled & Hot-Rolled | Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting |
Pipes / Tubes | Seamless Pipes/Tubes, Welded Pipes/Tubes | OD:6-219mm x WT:0.5-20.0mm | Hot extrusion, Cold Drawn, Welded | Annealed, Solution and Aging, Q+T, ACID-WASHED |
Grade | Standard | Country | Application |
---|---|---|---|
ЖC3-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC3ЛK-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC30-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC3-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC3ЛK-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC30-BИ | GOST | Russia | Russia GOCT Standard vacuum smelting casting high temperature alloy bar |
ЖC3 | GOST | Russia | Russia TY standard grades and chemical compositions of the high temperature alloy castings |
ЖC3ЛK | GOST | Russia | Russia TY standard grades and chemical compositions of the high temperature alloy castings |